This report was prepared as an account of work sponsored by an agency of the United States Government. Neither the United States Government nor any agency thereof, nor any of their employees, makes any warranty, express or implied, or assumes any legal liability or responsibility for the accuracy, completeness, or usefulness of any information, apparatus, product or process disclosed, or represents that its use would not infringe privately owned rights. Reference herein to any specific commercial product, process or service by trade name, trademark, manufacturer, or otherwise does not necessarily constitute or imply its endorsement, recommendation, or favoring by the United States Government or any agency thereof. The views and opinions of authors expressed herein do not necessarily state or reflect those of the United States Government or any agency thereof.
This report has been reproduced directly from the best available copy.
Available to DOE and DOE Contractors from the Office of Scientific and Technical Information, P. O. Box 62 Oak Ridge, TN 37831; prices available from (423) 576-8401.
Available to the public from the National Technical Information
Service, U.S. Department of Commerce, 5285 Port Royal Road, Springfield, VA
22161.
Storage of aluminun-clad spent nuclear fuel at the Savannah River Site (SRS)
and other locations in the U. S. and around the world has been a concern over
the past decade because of the long time interim storage requirements in water.
Pitting corrosion of production aluminum-clad fuel in the early 1990's at SRS
was attributed to less than optimum quality water and corrective action taken
has resulted in no new pitting since 1994.
The knowledge gained from the corrosion surveillance testing and other
investigations at SRS over the past 8 years has provided an insight into
factors affecting the corrosion of aluminum in relatively high purity water.
This paper reviews some of the early corrosion issues related to aluminum-clad
spent fuel at SRS, including fundamentals for corrosion of aluminum alloys. It
updates and summarizes the corrosion surveillance activities supporting the
future storage of over 15,000 research reactor fuel assemblies from countries
over the world during the next 15-20 years. Criteria are presented for
providing corrosion protection for aluminum-clad spent fuel in interim storage
during the next few decades while plans are developed for a more permanent
disposition.
Keywords: Aluminum-clad, pitting corrosion, Savannah River Site (SRS), IAEA,
Processing of aluminum-clad nuclear fuel was suspended at the Savannah River
Site (SRS) and other locations within the DOE Complex in late 1989 due to
safety upgrades and the U.S non-proliferation policy. Spent production fuel
normally stored in water-filled basins at SRS for 12-18 months while awaiting
processing, accumulated several years of exposure in less than optimum water
conditions. Pitting corrosion of the aluminum resulted in breach of the
cladding.1 Corrosion surveillance tests in the reactor storage
basins conducted over several years provided a basic understanding of the
mechanisms of corrosion.2-4 Recommendations were implemented to
improve basin water quality and as a result, no new pitting corrosion has been
seen since 1994. Today, with the restart of SRS canyon separations facilities,
most of the old production fuel has been processed and new shipments of foreign
and domestic research reactor spent fuel are being put into interim wet storage
in the L and RBOF basins at SRS.
The knowledge gained from the corrosion surveillance testing and other investigations at SRS over the past 8 years has provided an insight into factors affecting the corrosion of aluminum in relatively high purity water. This paper reviews some of the early corrosion issues related to aluminum-clad spent fuel at SRS and and provides fundamentals for corrosion of aluminum alloys. It updates and summarizes the corrosion surveillance activities which will continue to support the storage of over 15,000 research reactor fuel assemblies from countries over the world during the next 15-20 years. Criteria are presented for providing corrosion protection over the next few decades for aluminum-clad spent fuel in interim storage as plans are developed for a more permanent disposition.
Storage of spent fuel at SRS has been successful over the 50 years of plant
operations. Irradiated aluminum-clad production fuel has been stored in
water-filled basins connected to the P, K, and L-Reactors while awaiting
processing. Foreign and domestic research fuel has been traditionally stored
in the Receiving Basin for Off-Site Fuels (RBOF) basin. The water in these
basins is currently being maintained at a conductivity of 1-3 µS /cm using
mixed-bed, continuously operated deionizers.
Corrosion concerns on the spent fuel have been minimal over the years of fuel
storage. The water conductivity was maintained in the 60-70's µS /cm
range in the 1970 through late 1980's using portable mixed bed deionizers.
Some pitting was reported on aluminum-clad tritium target materials, but this
was attributed to material defects and fabrication concerns.
Over 200 Metric Tons Heavy Metal (MTHM) of aluminum-clad fuel and target
materials were stored in the basins at SRS in the early 1990's.5
The aluminum cladding alloys were 30-mil thickness and primarily Types 1100,
8001, and 6061. The core materials were generally depleted uranium metal or
uranium-aluminum alloys. With the suspension of processing and extended
storage times, nodular corrosion product became visible on the aluminum
cladding of Mk 22 assemblies in the K-Reactor basin and on the Mk 31A target
slugs in L-Reactor basin as shown by Figures 1-2. Sampling and analysis of the
corrosion products from the spent fuel cladding showed that cesium-137,
uranium, plutonium, and other fission products were present. The cesium level
was continuously monitored through water analysis and was continuously removed
by the mixed-bed deionizers. The cesium-137 level in the water was always
maintained well below the administrative limits set for the basins. The water
chemistry in the basins at the time when corrosion was most aggressive in the
basins showed the chloride ion concentration at 8-14 ppm and a conductivity of
160-175 µS /cm.
The factors believed to have played the most important role in the corrosion of aluminum-clad spent fuel in the reactor basins at SRS are:
The RBOF basin at SRS stores spent fuels from research reactors around the world. Corrosion of fuel in this basin has never been an issue over the 37 years of operations. In this basin, water purity is maintained by continuous mixed-bed deionization. Impurity concentrations are maintained in the parts-per-billion (ppb) range and the water conductivity is usually stable in the 1-3 µS /cm range. The cesium-137 levels in the RBOF basin are generally higher than in the reactor basins because of failed fuel from the research reactors around the world being stored in the basin.
The factors promoting the corrosion of aluminum are complex. In many cases, they operate synergistically. These factors, including fundamentals and mechanisms have been discussed in detail in a previous NACE paper.3 Some of the most important factors which affect the corrosion of aluminum alloys and aluminum-clad spent fuel are presented here for background to the criteria for protection.
Aluminum is one of the most thermodynamically reactive metals and owes its
excellent corrosion resistance to the protective oxide film formed and strongly
bonded to its surface. When the film is damaged under conditions that
self-healing does not occur, localized corrosion in the form of pitting or
intergrannular attack can occur.6 In water at temperatures about
60-70 0C, the amorphous barrier oxide on aluminum thickens with the
formation of the crystalline hydrated oxide phase, Boehmite
(Al2O3.H20). After days of
immersion the crystalline phase Bayerite
(Al2O3.3H20) is formed. At and
above 70 0C, the oxide films formed on aluminum are predominately
Boehmite.
The overall reaction for aluminum corrosion in water is given by the equation:
The major factors believed to influence the pitting of aluminum alloys are: conductivity, pH, bicarbonate, chloride, sulfate, and oxygen content.6 Because of the inter-relationship of the composition and service factors, it is difficult to predict the influence of the water from a table of water composition alone. A number of studies conducted in synthetic water containing several metal and salt ions alone and in combinations have found that the corrosion of aluminum was accelerated by combinations of salts of copper, chlorides, and bicarbonates, over single impurities.7-9
As most of the corrosion processes involving the aluminum-clad fuels in storage basins are electrochemical, and corrosion depends on the nature of the electrolyte. For basin water, the conductivity plays a key role in the flow of electrons and electrical current in the process. The amount of metal removed by corrosion is directly related to the current flow. By increasing the resistance of the water, the corrosion of the aluminum can be reduced. Very pure water has a high resistance to the flow of current and is much less corrosive than impure or natural waters. Conductivity is defined as reciprocal of specific resistivity:
Where the unit for C is 1/ohm-cm or mho/cm. A smaller popular unit is
µmhos/cm. In International Units, 1 µmhos/cm =1 µS/cm where S is
the unit Sieman.
Extremely pure water with a conductivity of less than 1 µS/cm can be produced by deionizaton for atomic energy purposes. Type 1 reagent-grade water can be produced by deionization, distillation, reverse osmosis, or combinations of these techniques to a conductivity level below 0.1 µS/cm. Natural lake waters in some areas such as Lake Ontario, Canada have a typical conductivity of about 270 µS/cm as compared to 40,000 µS/cm for seawater.10
Aluminum is passivated and protected by its oxide film in the pH range of about
4-8.5. The limits vary somewhat with temperature and the specific form of
oxide present, and with the presence of substances that can form soluble
complexes or insoluble salts with aluminum. The oxide coating is soluble at pH
values below 4 and above 8.5. General corrosion in distilled water at 60
0C has been shown minimum at pH4 rising slightly in the passive
range and faster between pH 9 and 10. For pitting corrosion, which is the
predominant mechanism for aluminum in water, the pitting potential in chloride
solutions has been found to be relatively independent in the range of
4-9.11 Godard indicated that a deviation from neutrality (pH7) on
both acid and alkaline sides could increase the rate of pitting in fresh
waters.
The corrosion rate is often more dependent on the specific ion that causes the pH than on the pH itself. For example, aluminum is not rapidly attacked by concentrated nitric acid at a pH of 1, or by glacial acidic acid at a pH of 3, but is rapidly corroded by hydrocloric or phosphoric acid at a pH of 4. On the alkaline side, aluminum is resistant to ammonium hydroxide at pH 13, but is corroded rapidly by sodium hydroxide at pH of 11. The probable reason for this behavior lies in the composition of the corrosion product and their tendency to form protective films on the aluminum surface.6
The rate of corrosion of aluminum alloys and their tendency for pitting is
controlled by the protective oxide film formed on the aluminum surface. The
corrosiveness of basin water is influenced to a large degree by the ability of
impurity ions to penetrate the oxide film and attack the aluminum metal.
Sverpa found that the penetrating power of anions in decreasing order to be
chloride, bromide, iodide, fluoride, sulfate, nitrate, and
phosphate.12
For aluminum, pitting corrosion is most commonly produced by the halide ions,
of which chloride (Cl-) is one of the frequently encountered. An
increase in the chloride concentration of a solution has been shown to decrease
the pitting potential of aluminum. Chloride breaks down the protective oxide
film and inhibits re-passivation. It stimulates the metal dissolution. It is
difficult to specify a chloride limit below which pitting corrosion does not
occur because of the synergistic reactions that take place with other anions in
the water.
Heavy metal ions such as copper and mercury are very aggressive toward the
pitting corrosion of aluminum alloys. The aluminum reduces the ions of copper,
mercury, lead, etc. These ions can plate out on the aluminum and form localized
galvanic cells with the aluminum becoming the anode and the heavy metal
becoming a very effective cathode.
Water hardness or softness as measured by the carbonate content is another
important factor in determining the aggressiveness of the water toward pitting
corrosion of aluminum. The bicarbonate ion alone, at concentrations up to
300-400 ppm has been shown not to pitting, but in combinations with chloride
and copper, calcium carbonate ions has led to intensive pitting.8-9
At low bicarbonate levels, voluminous corrosion products were dispersed in
solutions around the pits. With increased concentrations of bicarbonate,
harder, thicker caps of nodular corrosion products were formed which firmly
adhered to the pits.
Studies by Draley have shown that the presence of sulfate at 50 0C
and 70 0C reduces the corrosion rate of aluminum.13 The
sulfates decreased the oxide film thickness formed as the concentration of
sulfates increased. The thinner the film, the more susceptible the base metal
is to corrosion.
Surface waters and storage pools are normally saturated with oxygen, but if there were areas of a spent fuel storage pool where oxygen was reduced, it would likely diminish the corrosion rate of aluminum. Measurements of dissolved oxygen in the storage basins at SRS found the water to be saturated at 10.9 ppm and constant with depth.
In the wet storage of aluminum-clad spent nuclear fuel, there are a number of
corrosion mechanisms, which potentially come to play. The most important of
these as they pertain to the aluminum-clad alloys are discussed below.
General Corrosion. The general corrosion behavior of aluminum in high
purity water is very good. There is not a gradual thinning of aluminum as
occurs with steel and this mechanism has not been a problem in spent fuel
storage basins.
Galvanic Corrosion. Galvanic corrosion occurs when a metal or alloy is
electrically coupled to another metal, usually dissimilar, in the same
electrolyte. Galvanic corrosion is evident through fuel storage basins.
During galvanic coupling corrosion of the less corrosion resistant metal
increases and the surface becomes anodic, while corrosion of the more
corrosion-resistant metal decreases and the surface becomes cathodic. Factors
affecting galvanic corrosion are area ratios, distance between electrically
coupled alloys, and geometric shapes. Galvanic corrosion of the anodic metal
usually takes the form of general or localized corrosion.
Crevice Corrosion. Crevice corrosion of aluminum alloys is highly
localized corrosion occurring on closely fitted surfaces upon entry of water
into the crevice. The general theory is that s complex mechanism exists in
which chloride ions are drawn into the crevice as metal dissolution occurs and
acidic conditions exist. Aluminum, which depends on a passive film for
corrosion protection, is particularly susceptible to crevice corrosion.
Crevices between fuel hangers and fuel as well as in storage buckets and
storage racks form many possibilities for crevice corrosion to occur.
Pitting Corrosion. The primary mechanism for corrosion of aluminum-clad
fuel and target materials in wet storage in the U. S. and around the world has
been pitting. Pitting is a localized form of corrosion in which metal is
removed preferentially at point locations on the surface to develop cavities or
pits. The attack is generally limited to small areas while the remaining
surface is relatively unaffected. Pitting requires the presence of an
electrolyte and in the case of fuel storage basins, less than optimum deionized
water serves this purpose. Pitting is most common in metals that are covered
with an adherent film. The pits tend to develop at defects or flaws in the
surface of the film and at sites of mechanical damage where it is unable to
repair itself.
Pitting, like general corrosion has been shown to proceed by an electrochemical
process. The pitting is caused by electrochemical differences at two adjacent
locations at the metal-liquid interface. An individual pit is, therefore, a
local cell with its own anode and cathode.
The pitting can be described as an autocatalytic process. The corrosion
processes within a pit produce conditions that are both stimulating and
necessary for continuing activity of the pit. In a situation where metal is
being pitted by an aerated chloride-containing electrolyte, rapid dissolution
occurs within the pit, while oxygen reduction takes place on the adjacent
surfaces. The rapid dissolution within the pits tends to produce excess charge
in this area and results in the migration of chloride ions into the pit to
maintain neutrality. Thus in the pit, there is a high concentration of metal
chloride and a high concentration of hydrogen ions. As a result, the pits
become more acidic, reaching low pH levels and stimulating further dissolution
of most metals.
The rate of penetration of pits in aluminum decreases rapidly with time Aziz and Godard found that the pitting rate cure follows a cube-root law, given by:14
where d = maximum pit depth, t = time, and K = constant depending on the
particular alloy and the water conditions (composition, temperature, velocity,
etc.). One can see that doubling the wall thickness of the metal can increase
the time for perforation by a factor of eight.
The most undesirable result of pitting corrosion of spent fuel cladding is the perforation of the barrier material that protects the fuel core. This allows the release of the radioactive products such as uranium, plutonium, and cesium 137 to the basin water as the core corrodes. Build-up of this radioactivity in the basin water can ultimately lead to high radiation levels and exposure to personnel working around the basins.
Most of the Foreign Research Reactor and SRS production fuel and target
materials are clad with aluminum alloys, but the active core of the fuel is
uranium metal or a uranium-aluminum alloy. Once the 30-mil cladding (some
foreign fuels have 15-mil clad) is breached, the active core material is
exposed to water. The Mark 31A target slugs stored in the SRS basins had an
1100-aluminum alloy cladding and a uranium metal core. When the cladding was
breached during the first two years of storage, the corrosion continued into
the uranium metal core material producing voluminous uranium oxide corrosion
product as seen in Figure 1.
An excellent description of classical corrosion of uranium is provided by the work done in the late 1950's.15 In general, once the clad has been penetrated by pitting corrosion, the compounds formed by the nickel bonding layer between the aluminum and the uranium may become slightly anodic to the aluminum and result in undercutting of the cladding by galvanic corrosion when exposed to the basin water. When uranium is metallurgically bonded to aluminum by a material like nickel, it corrodes somewhat more rapidly than bare uranium, but the increase in rate is more than offset by the smaller, restricted area of attack. The good bonding minimizes exposure of the uranium to the water. The corrosion of uranium in water can be expressed by the reaction:
The corrosion can be divided into two stages: an initiation stage,
corresponding to the induction period observed in the corrosion of bare
uranium, and a propagation stage. The initiation stage usually is an
unpredictable length. There is generally absence of any significant swelling,
but occasional bubbles of hydrogen may be evolved, and the pinhole in the
aluminum may be discolored by small particles of UO2. The
propagation stage is characterized by the growth of a blister at the pinhole.
Once swelling starts, the blister grows at a fairly steady rate until the
accumulated uranium oxide causes the cladding to split. After the cladding
splits, the UO2 is released into the water and a larger area of the
metal is exposed to attack. If the uranium core is of sound metal and the bond
layer has no flaws or discontinuities, the blister is usually localized at the
pinhole and has a mountain-like profile.
If the uranium contains stringers of voids or rolling seams, diffusion paths
are provided for the hydrogen resulting from attack at the pinhole. Because of
the small diameter of such flaws in uranium, the hydrogen can diffuse through
them more rapidly than water, steam, or air. When the hydrogen encounters a
site susceptible to attack (not protected by oxide), uranium hydride can be
formed. This hydride attack is characterized by the appearance of a blister at
a distance from the original pinhole. Since uranium hydride forms rapidly and
has a lower density, the hydride blister almost always grows more rapidly than
the original blister at the pinhole in the cladding, and the cladding usually
splits first at the hydride blister. The splitting of the hydride blister
exposes uranium hydride to water, with the formation of UO2 and
hydrogen, and simultaneously exposes a large area of uranium to attack.
The uranium hydride attack is generally more rapid than the direct attack of
uranium by water.
The Mark 22 fuels used in the SRS reactors contained two concentric aluminum-clad fuel tubes using an enriched uranium-alloy core. This alloy core consisted primarily of particles of UAl3 and UAl4 embedded in an aluminum alloy matrix. The nominal distance between larger particles was generally in the range between 1.5 to 45µm (0.06-1.8 mil.) The particles were broken up after the extrusion process. Corrosion of this alloy based on preliminary electrochemical laboratory tests was found to be similar to an aluminum alloy, itself. The corrosion rate of 8001 aluminum was measured at about 0.175 mpy compared to 0.171 mpy for the UAl4 alloy.16 The release of cesium from this type fuel is expected to be much slower than that from uranium metal.
In order to develop a fundamental understanding of the corrosion problems with aluminum-clad spent fuel in the SRS wet storage basins in early 1992, a corrosion surveillance program was implemented. The program consisted of in-basin tests using corrosion surveillance coupons and laboratory electrochemical tests. Information obtained from these programs provided the basis for recommendations for improvements to plant equipment and basin operations to mitigate corrosion of the spent fuel.
These test were initiated in early 1992 after corrosion coupon scoping tests
indicated that water in the reactor basins was aggressive to the corrosion of
aluminum alloys used in the cladding for SRS fuel and target materials. Actual
un-irradiated fuel and target tubes from a Mark 22 fuel were cut into 6 inch
long cylinders and nested together like real fuel assemblies. The individual
fuel and target tubes were pre-oxidized in deionized water to give about
1-micron thickness of Boehmite phase oxide on the surfaces. A total of 6 nested
coupons were placed on a rack that could be lowered into the basin water at a
depth of 3-6 below the surface. After various exposure times, two coupons were
removed and metallography done on any pitting that was found. Two additional
nested coupons were added to the rack and re-immersed in the basin. Corrosion
racks were initially placed in the K-Reactor basin and expanded to L, P, and
RBOF by early 1994.
The Component Immersion Tests have continued from 1992-2000. Results of these withdrawals can be seen in Table 1. Coupons were withdrawn more frequently early in testing, as the basin water was more aggressive before positive steps were taken to mitigate the corrosion. Early withdrawals in K-basin during 1992 showed that pitting through the 30-mil clad occurred in as little as 45 days. At the time of this exposure, the water in K-basin had a conductivity of about 180 µS/cm with 8 ppm chlorides. With pitting very aggressive in K-basin and earlier scoping tests indicating that the other reactor basins were equally aggressive, immediate steps were taken to continuously deoinize all basins. With further deionization of the basins and conductivity levels lowered to the 100-125 µS/cm range, no pitting was seen in K and L-basins. With continuous deionization of the RBOF basin and the conductivity maintained in the 1-3 US/cm range, no pitting has ever been seen on corrosion surveillance coupons. When conductivity of the P-basin reached 165 µS/cm pitting re-appeared on fuel in that basin.
The L-Reactor basin at SRS was refurbished to receive a large number of the
aluminum-clad research reactor assemblies from both domestic and foreign
sources over the next 20 years. With this refurbishment, a comprehensive
corrosion surveillance program was developed to directly support the new
extended fuel storage activity at SRS. This program was initially for basin to
demonstrate that this storage basin could provide a suitable environment for
long term interim storage of aluminum alloys after the basin upgrades during
1994-1996. The RBOF basin, shown in Figure 3, with its superb water quality
over the years of operations and extremely low conductivity did not experience
the pitting corrosion problem seen in the reactor basins in 1992-1993.
However, the new surveillance program was implemented in this basin to provide
additional data to supplement the existing Component Immersion Program.
The Research Reactor Corrosion Surveillance Program was designed to support the
receipt of both domestic and Foreign Research Reactor (FRR) fuels. The
corrosion monitoring program concentrates on aluminum alloys that are typical
of cladding materials for spent foreign reactor fuel. Other alloy-clad fuels
like Zircaloy and stainless steel are likely to go to another DOE storage basin
in Idaho and are not included in this program. In addition to providing data
to support fuel receipts at SRS, results from this program feed directly into
the IAEA sponsored corrosion surveillance activities for research reactor
aluminum-clad spent fuels.
The testing for this program began in both L-Reactor basin and in RBOF in
January 1996. This was deemed adequate lead-time to determine the suitability
of the reactor basin water for the extended storage of the FRR aluminum-clad
materials. Data from this program and laboratory corrosion testing programs
provide a technical basis for maintaining and improving basin management
practices, establishing operational limits, and will aid in the prediction of
fuel storage performance in the basin.
Corrosion Racks and Test Coupons. The corrosion samples are 31.75 mm (1 1/4 in.) circular disks of 3.175 mm (1/8 in.) thickness with a hole in the center designed to fit over the insulated stainless steel rod rack. Plastic insulators separate individual samples. The coupons are not pre-oxidized at elevated temperature in water, but have the normal air formed oxide. This condition should make them more sensitive to any water chemistry changes. Four basic types of corrosion specimens are being tested in the L-basin and RBOF water environments:
Based on the current inventory of fuel in the RBOF basin and the available
information for incoming research reactor fuel, 1100, 6061, and 5086 aluminum
alloys are the primary cladding alloys expected to be stored in the basin.
Welded and galvanic samples will concentrate on the 1100 and 6061 alloys. Some
304L stainless samples are included in galvanic couple tests to represent
potential interactions that have typically existed over the years in most
storage basins around the world. Multiples of each type coupon are included on
each corrosion rack. Each rack contains 60 samples. A typical rack is shown
in Figure 4.
Schedule for Withdrawal and Analysis. Eighteen corrosion racks are
available for the SRS Research Reactor Corrosion Surveillance Program. Twelve
racks are immersed in two different areas of L-basin. Six racks are immersed
in the RBOF basin to support the program that is currently scheduled to last
for twenty years. The corrosion-monitoring program was designed to
provide data after six months, one year, two years, five years, ten years, and
twenty years of exposure. Duplicate racks are scheduled for examination at the
end of each pre-determined exposure time. The first three withdrawals up
through two years of exposure were designed to provide an early indication of
the aggressiveness of the storage environment on the aluminum coupons.
Along with color photography and metallurgical examination of the specimens, a detailed characterization of the basin water during the exposure period will be obtained from the existing water sampling and analysis program. The water conductivity, pH, chloride, nitrate, nitrite and sulfate content will be recorded.
Results. A total of six racks were withdrawn from the two basins
during 1996-1997. These racks were withdrawn after six and 12 month's
exposure. No pitting was observed except where embedded iron particles were
found on 4 specimens from polishing by the vendor.
Three additional racks were removed from L-basin and from RBOF in early 1998
after 2 years of exposure in water conditions that generally ranged from 1-3
µS/cm conductivity with a chloride ion content in the parts-per-billion
range. No pitting was observed on these racks. Some mild surface oxidation
was seen on all coupons. Some mild surface reaction was seen in the crevice
area of the stainless/aluminum galvanic couple samples.
A new simplified corrosion rack was designed in early 1999 to supplement the existing program. The new rack contained a reduced number of wafer samples of the aluminum alloys, with crevice and some galvanic samples. This rack was designed to be use to fill in the gaps for years in which there were no scheduled withdrawals in the original program. Fifteen additional racks were immersed in RBOF and L-Reactor basins in February 1999 and a new schedule for withdrawals made. The new schedule calls for a minimum of one withdrawal each year over the 20-year program.
With the aggressive nature of the water in K-Basin having been demonstrated by
the pitting corrosion of the coupons during the corrosion tests and by the
visual inspections of the fuel and target materials in the basins, a
concentrated basin cleanup effort was initiated in the basins during 1993.
Through a Basin Management Team consisting of reactor engineering, operations,
and SRTC technical personnel, extensive manpower and resources were devoted to
activities designed to improve basin storage conditions.
Based on initial observations and understanding on what was driving the
corrosion processes, recommendations were made to improve the water quality.
The effort initially started in the K-Basin with extensive deionization of the
basin water that had approached 180µS/cm. Using the portable mixed-bed
deionizers, the conductivity and impurity concentration of the water was slowly
lowered. K-basin conductivity reached as low as about 125 µS/cm by early
1995.
Extensive deionization occurred in L-basin during early 1994 reaching a low of
about 96 µS/cm from a high of over 160 µS/cm. The chlorides in this
basin were lowered from about 18 ppm to 11 ppm by the deionization. Due to
limited availability of deionizers, no special cleanup efforts were initiated
in P-basin until the conductivity reached about 165 µS/cm and some pitting
was seen on the aluminum corrosion surveillance coupons in that basin. After a
concentrated deionization campaign, the conductivity of the P-basin was lowered
to the 85 µS/cm range and no further pitting was seen. P-basin has
since been closed and all fuel transferred to the other basins.
In July 1995, a vendor was contracted to accelerate the deionization of the SRS
basins. Using mixed-bed deionization equipment that was installed in the
L-basin, the water conductivity was lowered from about 110 µS/cm to below
8 µS/cm in 2.5 months. After releasing the vendor deionizer to go to
K-basin, the SRS portable deionization equipment was used periodically to
further lower the conductivity to about 1.8 µS/cm by March 1996.
In October 1995, the vendor equipment was installed in the K-basin and by
February 1, 1996 all sections of the basin were down to a conductivity level
below 10 µS/cm. Westinghouse purchased the deionization equipment from the
vendor after the contract was completed. With continuous operation through
March, the conductivity was further reduced to the 2.5 µS/cm range. The
anion concentrations in the L and K-basins, typically chlorides, nitrates, and
sulfates, were reduced to about 0.5 ppm by the vendor deionization.
As part of the cleanup activities in the reactor basins, a Disassembly Basin
Upgrade (DBU) Project was initiated in 1994.5 This project
initially was to include three new permanent deionizers for the K and L-basins,
sludge removal from the basins, and new aluminum storage racks for L and
K-basins. The new DBU deionizer system began operating in both L and K-Areas on
June 3, 1996. The new systems are designed to operate continuously at a
flowrate of approximately 200 gpm through four vessels that are connected in
series. The first two vessels contain 50 cubic feet of mix-bed resin, the
third vessel holds 70 cubic feet of cation resin, and the final vessel contains
50 cubic feet of anion resin. With continuous deionization by the new DBU
system, the conductivity and chemistry of the L and K-basins is routinely
maintained at 1-3 µS/cm and is below 1 µS/cm for much of the time.
During 1994-1996 an extensive campaign of sludge removal was put into place.
Underwater vacuum cleaning equipment was developed and used to remove sludge,
several inches thick in some places, from the basin floor and other horizontal
surfaces. The sludge is predominately iron oxide, aluminum oxide and other
impurities which can set up localized anodic-cathodic sites on the aluminum
clad fuel. In addition, some of the impurities like chloride can be
concentrated several times the levels in the basin water.
The effort to clean up the basins has had a significant impact on the quality of spent fuel storage. With the basins routinely operating with a conductivity near 1 µS/cm and impurity concentrations in the ppb range, no new pitting corrosion has been seen on SRS fuel since 1994. In addition, fuel processing has been resumed at SRS and the worst of the old, corroded production fuel has been removed from the basins and reprocessed at this time.
Most of the fuel used in research reactors of eastern and western countries is
fabricated with a uranium-aluminum alloy core protected by an aluminum alloy
cladding material. A small percentage of the fuel is clad with stainless steel,
zirconium, or other alloys. Fuel is regarded as spent nuclear fuel (SNF)
regardless of burnup when it is discharged from the reactor core for the final
time. It is then normally placed in pools for cooling and interim storage
until a final disposition is made. Some of this aluminum-clad spent fuel has
been in water storage for more than 40 years and remains in pristine condition
while other fuel has been severely degraded by pitting corrosion. Pitting
corrosion of the fuel can lead to breach of the cladding material and release
of radioactivity to the storage basin. The criteria presented in this paper
provide guidelines for optimizing corrosion protection for aluminum-clad spent
nuclear fuel in wet storage pools and include recommended water chemistry,
operational practices, and other basin management techniques for extended
interim storage. The principles applied to obtain optimum water quality will
also result in low corrosion rates for the other cladding alloys used with
research reactor fuel.
Research reactor spent fuel is being stored in water filled basins around the world under a wide variety of storage conditions. Many of the pools have water purification equipment that maintains the water at high purity levels. In these basins, aluminum-clad fuels have been stored for 25-35 years without corrosion problems. Other storage pools are small and do not have high quality water. For these pools, corrosion of aluminum clad SNF has been a concern. As a part of the U.S. Department of Energy's decision to return foreign research reactor spent fuel to the United States, over 1700 aluminum-clad assemblies have been inspected for corrosion and mechanical damage.17 The condition of assemblies has ranged from pristine, with no visible corrosion, to severe and localized nodular corrosion with pitting. Approximately 7% of the assemblies inspected showed pitting, which was judged to be through the aluminum clad into the core of the fuel.
The corrosion of aluminum-clad spent nuclear fuel is dependent on a number of
interrelated factors. Many of the metallurgical factors are already inherent in
the spent fuel when the reactor operator receives the fuel from the fuel
fabricator for irradiation. Factors such as alloy composition, heat treatment,
microstructure; nature and thickness of the protective oxide coating,
inclusions and impurities in the alloy, and cold work play a role in the
corrosion process, but are not controllable during wet storage. The
recommended guidelines presented in this paper apply to the environmental and
service related factors that are normally controllable and can be used to
optimize the corrosion protection of the aluminum-clad fuel during interim wet
storage.
These guidelines are designed to prevent breach of this clad and subsequent
corrosion of the fuel core. Most of the research reactor fuel is fabricated
from uranium-aluminum alloy and this type of fuel exhibits a corrosion behavior
similar to aluminum. Therefore, implementation of these guidelines should also
minimize corrosion of the fuel core. The corrosion of a metallic uranium core
is a much more rapid chemical reaction than that for a uranium-aluminum alloy
fuel, but would still be reduced by implementation of these recommendations to
protect the aluminum clad.
Water Chemistry. Maintaining high quality water chemistry in the fuel
storage pool is the single most important factor in controlling corrosion of
aluminum-clad spent fuel assemblies and other aluminum components stored in the
pool. Treatment and purification of the water in the pool and any make-up
water through filters and using ion exchange resins is essential to achieving
optimum storage performance. The guidelines presented here provide the
recommended water parameters to minimize pitting and other forms of corrosion
on aluminum-clad spent fuel during extended interim wet storage:
Conductivity. The conductivity of the water in the fuel storage
basin shall be maintained as low as achievable and in the range of 1-3
µS/cm for optimum corrosion protection. This level may be
difficult to achieve in unlined pools. A level of 3-10 µS/cm may yield
satisfactory results provided impurities like chloride ions are in low
concentrations. There is some evidence that pitting may be suppressed below 50
µS/cm depending on other favorable conditions. Values near 200
µS/cm are known to be aggressive to pitting of aluminum.
pH. The pH shall be maintained in reactor pools in a range of 5.5 to
6.5. This pH level will minimize uniform corrosion. Pitting corrosion is
relatively independent over this pH range. Tight control of the pH is
essential for reactors that have the core and fuel storage basin sharing the
same cooling water. For away from reactor storage pools, a somewhat wider range
of 5.0-8.0 may be permissible. Irradiation is known to reduce the stability
range of the protective oxide and can result in extensive turbidity from
precipitation of aluminum hydroxide from the water.
Chloride (Cl). The chloride ion content of the water shall be
maintained as low as achievable and less than 1 ppm for optimum corrosion
protection. This level is generally achievable if water
conductivity is maintained in the 1-3 µS/cm range. Chloride ions
break down the passive film on aluminum and promote metal dissolution.
Sulfates (SO4). The total sulfate ion content of the water
shall be maintained at less than 1 ppm for optimum corrosion protection. However, for
unlined pools where chemistry is hard to control, a level at or below 10 ppm
should give satisfactory protection. An increase in sulfate concentration
results in a decrease in thickness of the protective oxide film with a
corresponding increase in the susceptibility to pitting corrosion.
Heavy Metals. The concentration of copper (Cu),
mercury (Hg), silver (Ag), and other heavy metal ions shall be
maintained at or below 0.02 ppm. Heavy metal ions are extremely aggressive to
the pitting corrosion of aluminum as they can plate out readily forming strong
galvanic cells. These ions have strong synergistic reactions with chloride,
bicarbonate, and calcium ions. Reduced metals in the basin sludge or
particulate in solutions can form galvanic cells leading to localized corrosion
when the particles are in contact with the aluminum.
Other Impurities. Impurity ions such as iron (Fe), aluminum (Al),
nitrates (NO3), nitrite (NO2) shall be maintained at
levels as low as possible. Normal deionization of the water in the storage
pool to 1-3 µS/cm should keep these impurities to the 1 ppm or
lower level. Any addition of cations or anions to the water increases the
water conductivity and offers less resistance to the flow of corrosion current
from the aluminum-clad.
Hardness. Maintain carbonate hardness of the water at 60 ppm or less
when possible. Carbonate (CO3-) and bicarbonate
ions (HCO3-) and can react synergistically with
chloride and copper and lead to intensive pitting of aluminum. Soft
water as defined by a carbonate content of 60 ppm or less is less
aggressive to aluminum corrosion than hard water at a carbonate content of 60
ppm or greater. Continuous deionization of the basin water softens the water
as it removes calcium carbonate and other ions contributing to the hardness.
Temperature. The water temperature shall be maintained at 40
0C or below. The rate of pitting at pitting at 40 0C has
been found to be 5 times the pitting rate at 25 0C. The density and
probability of pitting has been found to increase with temperature. The
corrosion rate of uranium metal increases dramatically with increasing
temperature.
Radiation Effects. Gamma radiation from irradiated fuel assemblies, cobalt-60 or radioactive cesium sources can have some effect on materials stored in fuel storage pools. The gamma fluxes, however, have little effect on the properties of the metal cladding and the radiation field does not seem to promote any significant increases in corrosion of the metals in wet storage. Gamma fields can deteriorate components subjected to radiolytic decomposition like neutron absorbers that include organic materials and rack configurations that trap water that subsequently forms gas pressure from radiolyic decomposition.
Water Circulation. Avoid stagnant areas of water in the fuel storage
basin. Ensure that the water is circulated to provide movement over the stored
fuel assemblies. As an example, a linear flow rate over the aluminum
surface as little as 2.4 meters per minute has been shown to suppress
pitting on some aluminum alloys.
Sludge Removal. Do not allow sludge to accumulate in the water of the
fuel storage basin. Remove on a periodic basis by vacuuming or other methods.
This material can concentrate chlorides, heavy metals, etc. and deposit on fuel
assemblies initiating pitting of the aluminum clad.
Filtration. Mechanical filters or resin beds shall be used to control
suspended solids or particulate material in the basin water before it turns
into sludge. Deionization of the water helps to accomplish this.
Skimmer System. Debris and other species floating on the water surface
of fuel storage pools shall be removed by a skimmer system or other means.
This material can settle on surfaces of fuel cladding and cause pitting
corrosion.
Crevices. Avoid crevices between the aluminum-clad assemblies and the
fuel storage racks or hangers. Low pH water conditions, concentration of
chloride ions, and oxygen concentration cells in these crevices can lead to
accelerated corrosion of the cladding.
Galvanic Couples. Avoid contact between aluminum-clad fuel assemblies
and dissimilar metal storage racks or hangers. Use aluminum storage racks or
provide non-conducting insulators whenever possible. Aluminum-clad fuel
coupled to stainless steel racks or hangers will accelerate pitting corrosion
of the aluminum.
Handling of Spent Fuel. Avoid handling fuel assemblies with
sharp edged tools as scratches in the oxide coating of irradiated fuel serve as
pitting initiation sites when in the storage basin. Minimize, as much as
possible, mechanical damage and surface scratches on fuel element surfaces
during discharge from the reactor core and during subsequent fuel handling and
storage operations.
Microbiological Activity. Do not add chemicals containing chlorides or
other halogens such as sodium hypochlorite (NaOCl) to the water in storage
basins for control of algae, bacteria, or turbidity without first testing for
compatibility with the fuel, basin lining, or other basin components. The
chloride in many of the chemicals will destroy the passive film on aluminum and
cause aggressive pitting corrosion.
Biofilm Formation at Air/Water Interface. The bath tub ring
often formed at the air/water interface around the sides of the basin is likely
a biofilm of microbial activity. This film acts like a trap and is known for
concentrating cesium and other radioactive isotopes contained in the basin
water. This biofilm should be removed mechanically by wet brushing using water
to hold down any airborne activity. A 35% solution (200mL in 700 gal) of
hydrogen peroxide (H2O2) has proven effective in killing
microbial activity and could be used to assist this removal without corrosive
attack on aluminum alloys.
Basin Lighting Conditions. The lighting conditions shall be maintained
as low as practical in and around the basin area. High levels of lighting
promote microbiological growth activity in the water. Ultraviolet lighting can
be used to suppress microbiological activity associated with filters, etc.
However, sidestream ultraviolet light systems are used primarily for planktonic
activity and are not effective on sessile colonies.
Make-up Water. Additions of water to the fuel storage pool should be of
a quality equal to or better than the existing pool water. Deionized water
shall be used whenever possible.
Radionuclide Activity in the Basin Water. Radionuclide activity
in the basin water leached from the spent fuel shall be monitored and
controlled to levels deemed to be safe for personnel working in the surrounding
area. Continuous deionization of the water removes alpha and beta-gamma
radioactivity from the water. Fission products such as Cesium-137 and other
radionuclides may be found in the water from the storage of failed spent fuel
elements or breach of clad. Special materials such as zeolite can be used in
the ion exchange type purification system to specifically target these
radionuclides for removal.
Water Sampling Plan. Maintaining water purity levels to the strict
guidelines presented here is vital for successful operation of a wet storage
fuel facility. Basin water quality is monitored through sampling, and trending
sampling results. All the major water parameters such as pH, conductivity, and
chlorides shall be measured on a periodic basis consistent with good basin
management practices. Weekly monitoring is recommended, but this interval can
be established by the basin operator and is dependent on pool conditions.
Other impurity ions such as sulfates, nitrates, nitrites, copper, mercury,
iron, and aluminum shall be measured quarterly as a minimum. Temperature shall
be monitored daily. The alpha and beta-gamma radioactivity measurements in
basins storing spent fuel shall be made on a frequency basis established by
individual requirements. An increase in radioactivity is an indicator of
corrosion. Permanent records shall be kept and analytical results trended.
A baseline evaluation of microbiological activity in the basin shall be made
from a sampling of the basin water. Analysis shall include counts of
hetrotrophic, acid producing, anaerobic, and sulfate reducing bacteria. This
baseline can be use to compare with analysis of bacteria at some later time.
Corrosion Surveillance Program. A long-term corrosion
surveillance program shall be implemented in the fuel storage pool to monitor
the aggressiveness of the basin water toward the corrosion of aluminum alloys.
Details for specific site programs can be tailored for the individual sites,
but should contain the generic elements described in this paper. A typical
program has been implemented in a number of countries with research reactor
fuel.18 Corrosion racks with coupons manufactured from aluminum
alloys typical of the spent fuel cladding shall be immersed in the water near
the stored aluminum-clad spent fuel. Standard corrosion coupons, either round
or rectangular shaped shall be used. Multiple coupons representing individual
aluminum alloys, crevice corrosion coupons, and galvanic coupons shall comprise
each rack. The coupons shall not be pre-oxidized other than air-formed oxide
normally found on the surface. This insures some conservatism.
A schedule for withdrawal of these coupons shall be formulated based on the
length of time fuel is expected to be in the basin and the total number of
corrosion racks available for testing. As a minimum there should be enough
racks available to obtain data after 6 months, one year, and two years to
provide an early indication of the aggressiveness of the storage environment on
the aluminum coupons. Depending on the expected storage life of the fuel, the
surveillance program should continue. For a twenty-year program, withdrawals
could be extended to 5 years, ten years, and twenty years exposure time. If the
water conditions are more aggressive, additional racks may be required and more
frequent intervals of withdrawal may be necessary. Ideally, however, enough
racks should be purchased to permit at least one withdrawal each year.
Metallographic evaluation of the corrosion coupons shall include pitting
density and maximum pit depth. Knowing pitting depth and exposure time, the
pitting rate may be calculated. Video and still color photography shall be
used to document the withdrawals. Data from the water analyses taken during
the exposure periods should be correlated with the corrosion observations on
the coupons to explain the test results.
Records Management Program. Data from the individual basin water chemistry and corrosion surveillance programs shall be maintained at the individual sites.
The storage of aluminum-clad spent nuclear fuel in less than optimum quality
water can result in aggressive pitting corrosion. This corrosion was a concern
at SRS in the early 1990's, but an aggressive Basin Management program resulted
in significantly improved storage conditions and no new pitting has been seen
in the reactor basins since 1994.
The knowledge learned from these basin cleanup activities and the corrosion surveillance program, underway since 1992, have provided a basic understanding of the important factors affecting the corrosion of aluminum-clad fuel. The criteria for corrosion protection of this fuel have been presented in this paper. Even though there are a number of important factors affecting this corrosion and some act synergistically, the key to improved and extended storage is based on improved water quality conditions. Improved water quality through continuous deionization results in low water conductivity and low impurity concentrations of important corrosion causing species like chloride ions. Aluminum-clad spent fuel can be stored safely and with minimum corrosion for times exceeding 25 years in water with a conductivity near 1 µS/cm and ppb quantities of impurities.
|
|||||||||
Basin |
Date |
Exposure (Days) |
Maximum Pit Depth (Mils) |
Pit
Density |
Avg. |
|
|
|
Avg. |
|
|
|
1100
8001 |
1100
8001 |
8 |
20 |
15 |
7.5 |
175 |
K |
6-92 |
75 |
13 45 |
0.125 .01 |
|||||
K |
3-92 |
107 |
23 39 |
0.125 .01 |
|||||
K |
6-92 |
182 |
58 27 |
0.125 .01 |
|||||
K |
12-92 |
365 |
100 57 |
0.125 .05 |
|||||
1993-2000 |
|||||||||
K |
3-94 |
65 |
No Pitting |
||||||
K |
7-94 |
181 |
|||||||
K |
2-95 |
403 |
6 |
18 |
9 |
7.3 |
125 | ||
K |
8-95 |
590 |
|||||||
K |
8-97 |
1091 |
|
<0.1 |
<0.1 |
<0.1 |
7.25 |
2.5 | |
L |
11-93 |
61 |
No Pitting |
||||||
L |
3-94 |
127 |
|||||||
L |
7-94 |
241 |
|||||||
L |
2-95 |
336 |
14 |
20 |
2 |
6.6 |
102 | ||
L |
8-95 |
340 |
|||||||
L |
8-97 |
1114 |
|
<0.1 |
<0.1 |
<0.1 |
6.6 |
1.8 | |
P |
11-93 |
61 |
No Pitting |
||||||
P |
3-94 |
127 |
|||||||
P |
7-94 |
241 |
|||||||
P |
2-95 |
336 |
35
mil Pits in 8001 |
10 |
9 |
18 |
7.5 |
160 | |
RBOF |
9-97 |
1222 |
No
Pitting |
0.1 |
6.19 |
1.18 | |||
RBOF |
8-95 |
480 |
No Pitting |
0.2 |
1.5 |
0.5 |
7.4 |
1 | |
RBOF |
4-96 |
723 |
No Pitting |
||||||